Metallographic Experiment for Laser welding of automobile lithiu

2022-10-22 17:07 作者:特魯利金相研究院  | 我要投稿

In the power battery system of new energy vehicles, the battery shell accounts for about 20-30% of the total weight of the system, and is the main structural part of the battery.Lightweight and high safety make aluminum alloy battery pack casings the mainstream of power battery casings.The?aluminum material used in power battery shell has the advantages of easy processing and forming, good high temperature corrosion resistance, good heat transfer and electrical conductivity.Therefore, the battery case with aluminum alloy is thinner and lighter than the steel case for the same capacity. In addition, once the battery explodes, the burst force of the aluminum case is also weaker than the steel case, and the harm caused by the aluminum shell power battery is relatively lower. At present, aluminum battery shells are mostly welded by laser.

?


?

01? ?Cutting

?

Cut the specimen with Beta-300Pro automatic cut-off?machine;

?


Beta-300Pro automatic cut-off?machine

?


?

Equipment

Beta-300Pro automatic cut-off?machine

Consumables

SiC?cutting?blade

Parameter

6a,0.6mm/s,2200rpm

02?mounting-?hot?mounting

?


Hot mounting with TJ2231 epoxy resin;

?

?MT-1H auto?mounting?press


?

?

Equipment

MT-1H?auto?mounting?press

Consumables

TJ2231

Parameter

180℃,120bar,5min, Medium-speed cooling

03? mounting-?cold?mounting

?


Cold mounting?with TJ2210 acrylic resin;




?ThetaMount cold?press

?

TJ 2210 Acrylic resin

?

?


?

?

Equipment

?ThetaMount?cold?press

Consumables

?TJ 2210 Acrylic resin

Parameter

0.3MPa,15min

04? ?Grinding?

?

?Grind the?specimen?with?GP-2000A automatic?grinder&polisher, abrasive?paper?P400→P2500;

?


GP-2000A automatic?grinder&polisher

abrasive?paper

?

?



Equipment

?GP-2000A?automatic?grinder&polisher

Consumables

?Abrasive?paper:P400;P800;P1200;P2000;P2500

Parameter

Pressure: 0.3MPa, upper speed:?80rpm, lower speed: 150rpm, time: 2min

05? ?Polishing - Rough Polishing

?

?Use GP-2000A automatic grinder&polisher?to polish the specimen, first use YS polishing cloth, with 3μm polycrystalline diamond suspension?for rough polishing while adding polishing lubricant.

?

?YS-JP white?fiber?polishing?cloth

?

?

?

?PD-W polycrystalline?diamond?suspension

?

Equipment

?GP-2000A?automatic?grinder&polisher

Consumables

YS polishing?cloth,3μm?polycrystalline?diamond?suspension,polishing?lubricants

Parameter

Pressure: 0.3MPa, upper speed:?80rpm, lower speed: 150rpm, time: 2min

06? ?Polishing-medium polishing

?

Use GP-2000A automatic grinder&polisher?to polish the specimen, and then use ET polishing cloth with 0.05μm alumina suspension in medium?polishing;

?



?ET-JP white?synthetic?velvet?polishing?cloth



?AO-P Alumina?suspension

?

Equipment

?GP-2000A?automatic?grinder&polisher

Consumables

?ET polishing?cloth,0.05μm?Alumina?suspension

Parameter

Pressure: 0.3MPa, upper speed:?80rpm, lower speed: 150rpm, time: 2min

?

07? ?Polishing - Fine polishing

?

Polishing the specimen with GP-2000A automatic grinder&polisher, then using ET polishing cloth with 0.05μm silicon dioxide suspension?for fine polishing;

?

?ET-JP white?synthetic?velvet?polishing?cloth

?

?

?

SO T401 silica?suspension

?

Equipment

GP-2000A?automatic?grinder&polisher

Consumables

?ET polishing?cloth,0.05μm?silica?suspension

Parameter

Pressure: 0.3MPa, upper speed:?80rpm, lower speed: 120rpm, time: 2min

08? Observation

?

?

?


Equipment

Leica DM2700M?metallographic?microscope

Consumables

?

Parameter

?50×→500× times observation

09? Analysis

?

?

?

?

??Right angle weld ?50×

?


? Right angle weld ?200×

?


?

?

?

???Fillet weld 50×

?


??Fillet weld 200×

?

There are gaps in the fillet?weld, so attention should be paid to cleaning the sample during grinding and polishing to prevent the leakage of the coarse particles contained and leave large scratches on the surface of the sample.

The sample preparation results?of cold mounting and hot mounting is the same.

Corrode?the?specimen?with?Keller's reagent.

Columnar crystals at the bottom of the laser weld pool, equiaxed grain in the core, lamellar segregation and holes are clearly visible.

?